304vs316L
304 (1.4301) and 316L (1.4404) are the two most common austenitic stainless steels. The difference is molybdenum: with 2.00–2.50% Mo and low carbon (≤ 0.030%), 316L resists chloride environments better. Chemistry, strength, welding and selection guide.
Chemical composition: where they differ
304 (EN 1.4301, X5CrNi18-10) and 316L (EN 1.4404, X2CrNiMo17-12-2) are the two most widely used austenitic stainless steels; the values on this page are based on EN 10088-3 for bar products. The key difference is molybdenum: 316L contains 2.00–2.50% molybdenum, while 304 has none. 316L also has more nickel (10.0–13.0% vs 8.0–10.5%), because molybdenum is a ferrite former and nickel is raised to keep the structure austenitic; its chromium is slightly lower (16.5–18.5% vs 17.5–19.5%). The second difference is carbon: the L in 316L stands for low carbon (at most 0.030%); for 304 the limit is 0.07%. The limits for manganese, silicon, phosphorus and sulphur are the same for both grades.
Chemical Composition
| Element | 304 | 316L |
|---|---|---|
| C | ≤ 0.07 | ≤ 0.030 |
| Si | ≤ 1.00 | ≤ 1.00 |
| Mn | ≤ 2.00 | ≤ 2.00 |
| P | ≤ 0.045 | ≤ 0.045 |
| S | ≤ 0.030 | ≤ 0.030 |
| Cr | 17.5–19.5 | 16.5–18.5 |
| Ni | 8.0–10.5 | 10.0–13.0 |
| Mo | — | 2.00–2.50 |
Heat (cast) analysis, % by mass.
Basis: 304 — EN 10088-3 · 1.4301316L — EN 10088-3 · 1.4404
—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).
Mechanical properties and strength
Mechanical values at room temperature are very close. To EN 10088-3, in the solution-annealed (+AT) condition and for diameters up to 160 mm, at least 190 MPa 0.2% proof strength is required for 304 and at least 200 MPa for 316L; tensile strength is 500–700 MPa for both. Elongation is at least 45% for 304 and at least 40% for 316L. In the annealed condition both grades are practically non-magnetic and keep their toughness at low temperatures. Both work-harden quickly during cold forming; 304 can partly transform to martensite with deformation and become slightly magnetic, while the higher nickel of 316L reduces this tendency. In short, the choice between these two grades is driven by corrosion resistance, not strength.
Mechanical Properties
| Property | 304 | 316L |
|---|---|---|
| Yield Strength (MPa) | ≥ 190 | ≥ 200 |
| Tensile Strength (MPa) | 500–700 | 500–700 |
| Elongation (%) | ≥ 45 | ≥ 40 |
Basis: 304 — +AT · d ≤ 160 mm · EN 10088-3316L — +AT · d ≤ 160 mm · EN 10088-3
Heat treatment and delivery conditions
Austenitic stainless steels cannot be hardened by heat treatment; strength can only be increased by cold working. The standard delivery condition is solution annealed and rapidly cooled (+AT), which dissolves carbides and gives the best corrosion resistance. This is where the carbon difference matters: if 304 spends a long time in the range of about 450–850 °C, for example when welding thick sections, chromium carbides can precipitate at the grain boundaries and create a risk of intergranular corrosion (sensitisation). The low carbon of 316L largely removes this risk. Solution annealing again after welding is often impractical, so low-carbon grades are preferred for welded applications in corrosive environments.
Weldability and machinability
Both grades weld very well and usually need no preheating. 304 is fine in thin sections; for thick, multi-pass welds, 304L (1.4307) or 316L is preferred because of the sensitisation risk. Welding 316L normally uses molybdenum-bearing filler metals of the 316L type. Both are harder to machine than carbon steels: because of work hardening they need sharp tools, adequate feed and plenty of coolant, and 316L is slightly more difficult to machine due to its higher nickel and molybdenum. For heavy machining there is the free-machining 303 (1.4305), but its corrosion resistance and weldability are lower.
Typical applications
304 is the general-purpose stainless steel: food and beverage equipment, kitchen and counter fabrication, architectural applications, storage tanks, indoor fasteners and general machine parts. 316L is used where chlorides, marine environments and chemicals are present: chemical and pharmaceutical plants, marine and coastal structures, water treatment, equipment for saline environments, heat exchangers, flanges, fittings and valves. In welded piping and pressure equipment, 316L is often chosen because of its low carbon.
Applications
- Food, beverage and dairy equipment (304)
- Chemical and pharmaceutical plants (316L)
- Marine and coastal applications (316L)
- Architectural and indoor applications (304)
- Flanges, fittings, valves and heat exchangers
304 or 316L: which to choose and when
If chlorides are absent or very low (indoors, dry atmosphere, clean water, most food applications), 304 is sufficient and more economical. Choose 316L where there is seawater splash, salt-laden air, chloride-bearing process water, swimming-pool atmospheres, acidic cleaning chemicals or welded thick sections. Resistance to pitting and crevice corrosion in chloride environments is roughly compared with the PREN (Cr + 3.3 Mo + 16 N): ignoring nitrogen, it comes to about 17.5–19.5 for 304 and about 23–27 for 316L. In hot, high-chloride environments both grades are susceptible to stress corrosion cracking; duplex stainless steels are then considered.
Equivalence caveats and ordering notes
These two grades are not equivalents of each other but different grades of the same family: 316L can replace 304 in most cases, but 304 cannot replace 316L. Name confusion is common: the EN counterpart of 304 is 1.4301 and of low-carbon 304L is 1.4307; 316 corresponds to 1.4401 and 316L to 1.4404, the higher-molybdenum variant is 1.4432, and the variant often requested by the pharmaceutical industry is 1.4435. ASTM and EN ranges do not match exactly either; for example, ASTM A240 allows 2.00–3.00% molybdenum for 316L, while EN 1.4404 is limited to 2.00–2.50%. Dual-certified 304/304L and 316/316L material is common on the market; check the inspection certificate (EN 10204 3.1) for which standards and grades are met, the heat analysis and the delivery condition.
Grade Equivalents
| System | 304 | 316L |
|---|---|---|
| EN | X5CrNi18-10 | X2CrNiMo17-12-2 |
| DIN (W.Nr.) | 1.4301 | 1.4404 |
| AISI / UNS | 304 / S30400 | 316L / S31603 |
| JIS | SUS304 | SUS316L |
| GB (China) | 06Cr19Ni10 | 022Cr17Ni12Mo2 |
Standards
304
- EN 10088-2
- EN 10088-3
- ASTM A240
- ASTM A276
- ASTM A182 F304
316L
- EN 10088-2
- EN 10088-3
- ASTM A240
- ASTM A276
- ASTM A182 F316L
The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.
Products made in these grades
- Stainless Steel BarsStainless Steel Round Bar
- Stainless Steel BarsStainless Steel Hexagon Bar
- Stainless Steel BarsStainless Steel Square Bar
- Stainless Steel BarsStainless Steel Flat Bar
- FlangesWeld Neck Flange
- FlangesSlip-On Flange
- FlangesBlind Flange
- FlangesThreaded Flange
- Pipe Fittings90° Elbow
- Pipe FittingsTee Fitting
Looking for this steel grade?
Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.