A105vsP250GH
ASTM A105 and EN P250GH (1.0460) are two carbon steels for forged flanges and fittings, but they belong to different design codes. A105: Rm ≥ 485 MPa, Re ≥ 250 MPa, ≤ 187 HB. Chemistry, heat treatment, temperature and selection notes.
Chemical composition: where they differ
A105 is the forged carbon steel for piping components (flanges, fittings, valve parts) covered by ASTM A105/A105M; P250GH (1.0460) is the non-alloy steel with specified elevated-temperature properties defined in EN 10222-2 for pressure-equipment forgings, and it corresponds to the former C22.8 of DIN 17243. A105 allows at most 0.35% carbon, 0.60–1.05% manganese, 0.10–0.35% silicon, at most 0.035% phosphorus and at most 0.040% sulphur; copper, nickel, chromium, molybdenum and vanadium are each limited, and their sum may not exceed 1.00%. The chemical limits of P250GH are not tabulated on this page; take them from the current edition of EN 10222-2 and from the material's inspection certificate.
Chemical Composition
| Element | A105 |
|---|---|
| C | ≤ 0.35 |
| Si | 0.10–0.35 |
| Mn | 0.60–1.05 |
| P | ≤ 0.035 |
| S | ≤ 0.040 |
| Cu + Ni + Cr + Mo + V | ≤ 1.00 |
Heat (cast) analysis, % by mass.
Basis: A105 — ASTM A105/A105M
Chemical and mechanical limits for P250GH are not tabulated on this page; take them from the current edition of EN 10222-2 and from the material's inspection certificate (EN 10204 3.1).
Mechanical properties and strength
ASTM A105/A105M requires for A105 at least 485 MPa tensile and at least 250 MPa yield strength, at least 30% reduction of area and at most 187 HB hardness; elongation is at least 22% on a round specimen with a 4D gauge length. Impact testing is not mandatory for A105; for low-temperature service it is either ordered as a supplementary requirement or a grade with an impact requirement, such as ASTM A350 LF2, is used. EN 10222-2, by contrast, gives the mechanical values of P250GH by thickness range and does not stop at room temperature: the 0.2% proof strength at elevated temperature and impact energy at a specified temperature are also part of the standard. In the EN 10027-1 designation system, P denotes steel for pressure purposes, the following number the specified minimum yield strength (MPa) for the smallest thickness range, and GH that elevated-temperature properties are specified. Exact thickness-dependent values must be read from the standard and the inspection certificate.
Mechanical Properties
| Property | A105 |
|---|---|
| Tensile Strength (MPa) | ≥ 485 |
| Yield Strength (MPa) | ≥ 250 |
| Elongation (%) | ≥ 22 (L0 = 4D) |
| Hardness (HB) | ≤ 187 |
Basis: A105 — ASTM A105/A105M
Chemical and mechanical limits for P250GH are not tabulated on this page; take them from the current edition of EN 10222-2 and from the material's inspection certificate (EN 10204 3.1).
Heat treatment and delivery conditions
When A105 forgings are heat treated, ASTM A105 provides for one of annealing, normalising, normalising and tempering, or quenching and tempering; for flanges above certain pressure classes and sizes, heat treatment is mandatory. P250GH forgings are mostly delivered normalised (+N) to EN 10222-2. In both steels the aim is a fine, uniform ferrite-pearlite structure that secures toughness and weldability; they are not used for hardening. Welded joints may require post-weld heat treatment depending on the design code and wall thickness.
Weldability and machinability
Both steels are designed for welding and are widely used in flange-to-pipe butt welds. Because carbon in A105 can reach 0.35%, the carbon equivalent varies from heat to heat; for thick sections the need for preheating must be determined from the actual analysis and the welding procedure specification (WPS). Some project specifications additionally impose a maximum carbon equivalent on A105. Machining is straightforward for both grades; flange and gasket faces are machined by standard methods.
Typical applications
A105 is the standard carbon-steel material for ASME B16.5 and B16.47 flanges, ASME B16.11 forged fittings (socket-weld and threaded), branch connections such as weldolets and sockolets, and valve body parts; it is used in oil, gas, petrochemical and power plants. P250GH is preferred for EN 1092-1 flanges and for boiler, pressure-vessel and pipeline forgings within the scope of the European Pressure Equipment Directive (PED).
Applications
- ASME B16.5 / B16.47 and EN 1092-1 forged flanges
- Socket-weld and threaded forged fittings
- Weldolets, sockolets and branch connections
- Valve body and bonnet parts
- Forgings for pressure vessels and pipelines
A105 or P250GH: which to choose and when
The design code decides: plants designed to ASME flange standards and piping codes such as ASME B31.3 use A105, while plants designed to EN 1092-1 flanges and European pressure-equipment standards such as EN 13445 or EN 13480 use P250GH. Using one grade instead of the other is a material substitution that affects the pressure-temperature rating, so it must not be done without the approval of the designer and, where required, the notified body. For low-temperature service, ASTM A350 LF2 is considered instead of A105; where higher strength is needed, grades such as P280GH or P305GH are considered on the EN side.
Equivalence caveats and ordering notes
A105 and P250GH are often called equivalent, but they are really two separate materials with similar fields of use: chemistry, mechanical values, heat treatment, testing and inspection requirements are defined in different standards and with a different logic. Dual-certified flanges meeting both standards are available on the market; in that case, the inspection certificate (EN 10204 3.1) must show that the requirements of each standard are met separately. For equipment within the scope of the PED, the material certificate must also satisfy the relevant requirements. In the order, state the product standard (for example ASME B16.5 or EN 1092-1), the material standard and grade, the pressure class, the size and, if needed, impact testing and additional inspections.
Grade Equivalents
| System | A105 | P250GH |
|---|---|---|
| ASTM / ASME | A105 / SA-105 | — |
| EN | — | P250GH |
| DIN (W.Nr.) | — | 1.0460 |
| DIN 17243 | — | C22.8 |
Standards
A105
- ASTM A105/A105M
- ASME SA-105
- ASME B16.5
- ASME B16.11
P250GH
- EN 10222-1
- EN 10222-2
- EN 1092-1
- EN 10273
The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.
Looking for this steel grade?
Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.