34CrNiMo6vs4340
EN 34CrNiMo6 (1.6582) and SAE 4340 are Ni-Cr-Mo quenched and tempered steels for the same jobs, but their chemistry differs: 4340 has C 0.38–0.43% and Ni 1.65–2.00%, 34CrNiMo6 has C 0.30–0.38% and Cr 1.30–1.70%. Strength, heat treatment and selection.
Chemical composition: where they differ
34CrNiMo6 (1.6582) is a nickel-chromium-molybdenum quenched and tempered steel to EN 10083-3 (now EN ISO 683-2); 4340 is the nickel-chromium-molybdenum steel defined in SAE J404 and ASTM A29. Both serve the same purpose, high strength and toughness in large sections, and are often named as each other's counterpart, yet their chemistry differs clearly. 4340 has more carbon (0.38–0.43% vs 0.30–0.38%) and more nickel (1.65–2.00% vs 1.30–1.70%). 34CrNiMo6, on the other hand, carries roughly twice the chromium (1.30–1.70% vs 0.70–0.90%). Molybdenum is similar in both (0.15–0.30% and 0.20–0.30%). EN caps phosphorus at 0.025% and sulphur at 0.035%; A29 allows 0.035% and 0.040%.
Chemical Composition
| Element | 34CrNiMo6 | 4340 |
|---|---|---|
| C | 0.30–0.38 | 0.38–0.43 |
| Si | ≤ 0.40 | 0.15–0.35 |
| Mn | 0.50–0.80 | 0.60–0.80 |
| P | ≤ 0.025 | ≤ 0.035 |
| S | ≤ 0.035 | ≤ 0.040 |
| Cr | 1.30–1.70 | 0.70–0.90 |
| Mo | 0.15–0.30 | 0.20–0.30 |
| Ni | 1.30–1.70 | 1.65–2.00 |
Heat (cast) analysis, % by mass.
Basis: 34CrNiMo6 — EN 10083-3 / EN ISO 683-24340 — SAE J404 / ASTM A29
Mechanical properties and strength
EN 10083-3 gives values for 34CrNiMo6 in the quenched and tempered (+QT) condition for sections up to 250 mm: up to 16 mm at least 1000 MPa yield and 1200–1400 MPa tensile strength, 16–40 mm at least 900 MPa and 1100–1300 MPa, 40–100 mm at least 800 MPa and 1000–1200 MPa, and 160–250 mm at least 600 MPa and 800–950 MPa. That values are defined for such large sections reflects the grade's high hardenability. SAE J404 and ASTM A29 define only the chemistry of 4340; its mechanical values follow the ordered heat treatment, the product standard or the specification. The higher carbon of 4340 reaches higher hardness and strength at the same tempering temperature; the lower carbon of 34CrNiMo6 is an advantage for toughness and welding.
Mechanical Properties
| Property | 34CrNiMo6 | 4340 |
|---|---|---|
| Yield Strength (MPa) | ≥ 900 | — |
| Tensile Strength (MPa) | 1100–1300 | — |
| Elongation (%) | ≥ 10 | — |
Basis: 34CrNiMo6 — +QT · 16 < d ≤ 40 mm · EN 10083-34340 — SAE J404 / ASTM A29
—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).
Heat treatment and delivery conditions
Both steels are used hardened and tempered. For 34CrNiMo6, typical practice is oil quenching from about 830–860 °C and tempering at 540–660 °C; 4340 is likewise oil hardened from a similar austenitising range. Thanks to their high hardenability, both harden through to the core in heavy sections, but for the same reason the risk of distortion and internal stress is high, so large forgings need controlled heating and cooling. Machining is usually done in the soft-annealed (+A) condition, followed by quenching and tempering. In some applications 4340 is tempered at low temperature for very high strength; toughness and susceptibility to hydrogen embrittlement must then be assessed separately.
Weldability and machinability
Because of their high carbon equivalent, both grades are difficult to weld: if welding is needed, high preheat, low-hydrogen filler, controlled cooling and post-weld heat treatment are mandatory. They are therefore mostly used as forged and machined parts rather than welded ones; the higher carbon of 4340 increases the risk of weld cracking. Machining is easiest in the soft-annealed condition; the high hardness in the quenched and tempered condition calls for carbide or coated tools and low cutting speeds. For heavy forgings, ultrasonic testing is frequently required to reveal internal discontinuities.
Typical applications
Both grades are used for heavy-duty parts: large-diameter shafts, crankshafts, turbine and compressor shafts, heavy gears, high-strength bolts, landing gear and structural aircraft parts, hydraulic and mining equipment. 34CrNiMo6 is common in European power-generation and heavy-machinery forgings; 4340 is a standard choice in US aerospace, defence and oil and gas equipment. In aerospace, 4340 is usually ordered to separate specifications such as AMS, together with cleanliness and melting-practice requirements.
Applications
- Large-diameter shafts and crankshafts
- Turbine and compressor shafts
- Heavy-duty gears
- Landing gear and structural aircraft parts
- High-strength bolts and forgings
34CrNiMo6 or 4340: which to choose and when
If the drawing is based on EN and a balance of toughness and strength in large sections is needed, choose 34CrNiMo6; US drawings, aerospace and API-based specifications call for 4340. Because the chemistries differ, substituting one for the other requires the heat-treatment parameters and target hardness to be re-validated: the higher carbon of 4340 gives a harder result at the same tempering temperature. For lower loads and medium sections, 42CrMo4 or 4140 is usually sufficient and more economical; for even larger sections, higher-alloyed EN grades such as 30CrNiMo8 are considered.
Equivalence caveats and ordering notes
34CrNiMo6 and 4340 are two grades of the same application class, but they are not chemical equivalents: their chromium ranges do not overlap at all, and their carbon ranges meet only at the 0.38% limit. A single heat therefore cannot meet both standards. The British BS 970 817M40 (EN24) is also close to this group and is often quoted as the counterpart of 4340. When switching grades, do not go by the name alone; assess the required yield and tensile strength, impact energy, section diameter and, if needed, the hardenability curve together. The inspection certificate (EN 10204 3.1) should show the heat analysis, the heat-treatment condition and the mechanical test results; for forgings, the ultrasonic testing requirement should be written into the order separately.
Grade Equivalents
| System | 34CrNiMo6 | 4340 |
|---|---|---|
| EN | 34CrNiMo6 | — |
| DIN (W.Nr.) | 1.6582 | — |
| AISI/SAE | ≈ 4340 | 4340 |
| UNS | — | G43400 |
| BS 970 | ≈ 817M40 (EN24) | ≈ 817M40 (EN24) |
| JIS | — | ≈ SNCM439 |
| GB (China) | — | ≈ 40CrNiMoA |
Standards
34CrNiMo6
- EN 10083-3
- EN ISO 683-2
- EN 10250-3
4340
- SAE J404
- ASTM A29/A29M
- ASTM A322
- AMS 6414 / AMS 6415
The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.