C45vs1045

EN C45 (1.0503) and AISI 1045 are close medium-carbon counterparts: carbon is almost the same (0.42–0.50% / 0.43–0.50%), but Mn, P-S limits and mechanical requirements differ. Chemistry, Q&T strength, welding and selection.

Chemical composition: where they differ

C45 (1.0503) is a non-alloy quenched and tempered steel to EN 10083-2 (now EN ISO 683-1); 1045 is the medium-carbon steel defined in SAE J403 and ASTM A29. Their carbon ranges are almost the same (0.42–0.50% vs 0.43–0.50%), so both grades have practically the same hardening potential. The differences are in the details: 1045 has slightly more manganese (0.60–0.90% vs 0.50–0.80%). C45 allows at most 0.045% phosphorus and sulphur; A29 allows up to 0.040% phosphorus and 0.050% sulphur. EN also limits residual chromium, molybdenum and nickel (together at most 0.63%), while A29 specifies silicon through ranges selected in the order. EN also offers C45E (1.1191) with tighter P and S limits and C45R (1.1201) with a controlled sulphur range.

Chemical Composition

ElementC451045
C0.42–0.500.43–0.50
Si≤ 0.40—
Mn0.50–0.800.60–0.90
P≤ 0.045≤ 0.040
S≤ 0.045≤ 0.050
Cr + Mo + Ni≤ 0.63—

Heat (cast) analysis, % by mass.

Basis: C45 — EN 10083-2 / EN ISO 683-11045 — SAE J403 / ASTM A29

—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).

Mechanical properties and strength

EN 10083-2 gives section-dependent mechanical values for C45. In the normalised (+N) condition, at least 340 MPa yield and 620 MPa tensile strength are required up to 16 mm. In the quenched and tempered (+QT) condition, it delivers at least 490 MPa yield and 700–850 MPa tensile up to 16 mm, at least 430 MPa and 650–800 MPa for 16–40 mm, and at least 370 MPa and 630–780 MPa for 40–100 mm. SAE J403 and ASTM A29 define only the chemistry of 1045; mechanical values depend on product form (hot-rolled or cold-drawn), heat treatment and order requirements, which is why the 1045 column of the table is empty. With the same heat treatment, the two steels give similar values. Their common limitation is hardenability: being non-alloy, only the zone near the surface hardens fully in thick sections, while the core stays softer.

Mechanical Properties

PropertyC451045
Yield Strength (MPa)≥ 430—
Tensile Strength (MPa)650–800—
Elongation (%)≥ 16—

Basis: C45 — +QT · 16 < d ≤ 40 mm · EN 10083-21045 — SAE J403 / ASTM A29

—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).

Heat treatment and delivery conditions

Typical practice is quenching in water or polymer from about 820–860 °C, followed by tempering at 550–660 °C; thin sections can also be oil hardened. EN defines the delivery conditions +A (soft annealed), +N (normalised) and +QT (quenched and tempered); in the USA, 1045 is mostly ordered hot-rolled, cold-drawn or annealed. Flame or induction surface hardening is a classic treatment for both grades, combining a hard, wear-resistant surface with a tough core. In water quenching, the risk of cracking rises at section changes and sharp corners, so part design must take this into account.

Weldability and machinability

Because of their medium carbon content, both grades have limited weldability: thin sections weld without trouble, while thick sections call for preheating (typically 150–250 °C) and slow cooling; surface-hardened zones should not be welded. Machinability is good in the normalised or annealed condition; for high-volume turning, grades with controlled sulphur such as C45R or, on the US side, the resulphurised 1145 improve chip breaking. Cold-drawn 1045 and bright C45 bar can be used directly for shafts and pins with tight tolerances.

Typical applications

C45 and 1045 are the most widespread and economical materials for medium-duty machine parts: shafts, axles, pins, bolts, gears, couplings, hydraulic piston rods and slideways. Induction-hardened shafts and bearing surfaces are also typical applications. For forged flanges or pressure equipment, however, materials defined in pressure standards (for example A105 or P250GH) are used instead of these grades.

Applications

  • Shafts and axles
  • Pins, bolts and couplings
  • Medium-duty gears
  • Hydraulic piston rods
  • Induction-hardened slideways and bearing surfaces

C45 or 1045: which to choose and when

If the drawing is based on EN, order C45 (or C45E with tighter P and S limits); US drawings and ASTM specifications call for 1045. Since the chemistries overlap widely, substitution rarely causes technical problems; but because mechanical values are defined in the standard for EN and in the order for A29, acceptance criteria must be written clearly into the order. As the section grows or high core strength is required, non-alloy steel reaches its limit; at that point chromium-molybdenum steels such as 42CrMo4 or 4140 are considered. If a lower-carbon material that welds more easily is needed, C35 or C22E can be considered.

Equivalence caveats and ordering notes

C45 and 1045 are among the closest counterparts, and their chemistries overlap over a wide area; most heats can satisfy both standards. Still, the lower manganese limit (0.50% for C45, 0.60% for 1045), the sulphur limit and the way silicon is specified differ. The name CK45 is the old DIN 17200 designation and corresponds today to C45E; JIS S45C and GB 45 are also close but separate standards. For dual-certified material, check that the inspection certificate (EN 10204 3.1) shows the heat analysis within both ranges and states the required delivery condition (+N, +QT or cold-drawn).

Grade Equivalents

SystemC451045
ENC45≈ C45
DIN (W.Nr.)1.0503≈ 1.0503
AISI/SAE≈ 10451045
UNS—G10450
JIS≈ S45C≈ S45C
GB (China)≈ 45≈ 45

Standards

C45

  • EN 10083-2
  • EN ISO 683-1
  • EN 10277

1045

  • SAE J403
  • ASTM A29/A29M
  • ASTM A576
  • ASTM A108

The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.

Request a Quote