S235JRvsA36
EN S235JR (1.0038) and ASTM A36 are close but not identical: A36 yield ≥ 250 MPa vs ≥ 235 MPa for S235JR; A36 allows more carbon and has no CEV limit or mandatory impact test. Chemistry, properties and how to choose.
Chemical composition: where they differ
S235JR is a non-alloy structural steel to EN 10025-2; A36 is the carbon structural steel of ASTM A36/A36M. Both are general-purpose weldable steels, but their chemical limits follow a different logic. For S235JR the heat analysis allows at most 0.17–0.20% carbon depending on thickness, 1.40% manganese, 0.035% phosphorus and sulphur and 0.012% nitrogen, and the standard also caps the carbon equivalent (CEV). For A36 the carbon limit is 0.25–0.29% depending on product and thickness; thin plate has no manganese requirement, thicker plate calls for 0.80–1.20%. Phosphorus is limited to 0.04% and sulphur to 0.05%, and there is no CEV limit.
Chemical Composition
| Element | S235JR | A36 |
|---|---|---|
| C | ≤ 0.17–0.20 | ≤ 0.25–0.29 |
| Mn | ≤ 1.40 | — (t ≤ 20 mm) · 0.80–1.20 |
| Si | — | ≤ 0.40 |
| P | ≤ 0.035 | ≤ 0.04 |
| S | ≤ 0.035 | ≤ 0.05 |
| N | ≤ 0.012 | — |
| CEV | ≤ 0.35 (t ≤ 40 mm) | — |
Heat (cast) analysis, % by mass.
Basis: S235JR — EN 10025-2A36 — ASTM A36/A36M
—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).
Mechanical properties and strength
On paper A36 is slightly stronger: it requires a minimum yield strength of 250 MPa and a tensile strength of 400–550 MPa. S235JR requires at least 235 MPa yield up to 16 mm, stepping down with thickness (225 MPa at 16–40 mm), and 360–510 MPa tensile strength from 3 to 100 mm. Elongation values cannot be compared one to one: EN uses a proportional gauge length (L0 = 5.65√S0), A36 uses 200 mm and 50 mm gauge lengths. The key difference is toughness: the "JR" in S235JR means at least 27 J Charpy V-notch impact energy at +20 °C, while A36 is impact tested only when this is ordered as a supplementary requirement.
Mechanical Properties
| Property | S235JR | A36 |
|---|---|---|
| Yield Strength (MPa) | ≥ 235 (t ≤ 16 mm) | ≥ 250 |
| Tensile Strength (MPa) | 360–510 | 400–550 |
| Elongation (%) | ≥ 26 (L0 = 5.65√S0) | ≥ 20 (L0 = 200 mm) |
| Impact Energy (J) at 20 °C | ≥ 27 | — |
Basis: S235JR — +AR / +N · EN 10025-2A36 — ASTM A36/A36M
—: the designation sets no value for this property, or no comparable value is given here. The binding value follows the product standard, the delivery condition and the order, and is stated on the inspection certificate (EN 10204 3.1).
Heat treatment and delivery conditions
Neither steel gets its strength from heat treatment; strength comes from chemistry and rolling, and neither is intended for hardening or quenching and tempering. S235JR is usually delivered as-rolled (+AR) or normalized / normalized-rolled (+N). A36 does not prescribe a delivery condition, and material normally arrives as-rolled. Welded structures can be stress-relieved, which lowers residual stresses but does not raise strength. Both grades are easy to cold-bend and form.
Weldability and machinability
Both grades weld well. The low carbon of S235JR and the CEV ceiling in its standard make preheat requirements easier to predict in thick sections. Because A36 may carry up to 0.29% carbon and has no CEV limit, welding procedures for heavy parts should be based on the actual heat analysis. In machining both are soft and ductile and form long chips; for high-volume turning a free-cutting steel is more productive.
Typical applications
These two grades are the workhorses of steel construction: connection and base plates, brackets, handrails, platforms, pipe supports, machine frames and general welded fabrication. They are the most common grades for flat bars, angles, sections and round bars. Where higher loads or low service temperatures are expected, designers move to the S355 class or to sub-grades with guaranteed toughness.
Applications
- Welded steel structures
- Base and connection plates
- Brackets, platforms and handrails
- Pipe supports
- Machine frames and general fabrication
S235JR or A36: which to choose and when
If the project is designed to Eurocode and EN 1090 and needs CE-marked fabrication, choose S235JR (or J0/J2 for lower temperatures). AISC/ASME drawings and US-origin specifications call for A36. The 250 MPa yield of A36 sits between S235 and S275; S275JR requires at least 275 MPa yield and 410–560 MPa tensile strength. So when an EN material is needed in place of A36, S275JR is often the closer match, and when A36 replaces S235JR, the impact requirement has to be checked separately.
Equivalence caveats and ordering notes
S235JR and A36 are close counterparts but not exact equivalents: carbon, phosphorus and sulphur limits, yield strength, the elongation test method and the impact requirement all differ. Dual-certified material meeting both standards is available on the market; when buying it, check that the inspection certificate (EN 10204 3.1) shows the test results for each standard separately. State the standard, grade, thickness or diameter, delivery condition and, if needed, the impact test temperature in the order. The old DIN name St 37-2 and JIS SS400 are only approximate counterparts.
Grade Equivalents
| System | S235JR | A36 |
|---|---|---|
| EN | S235JR | — |
| DIN (W.Nr.) | 1.0038 | — |
| DIN 17100 | St 37-2 | — |
| ASTM / UNS | — | A36 / K02600 |
| JIS | ≈ SS400 | ≈ SS400 |
| GB (China) | ≈ Q235B | ≈ Q235B |
Standards
S235JR
- EN 10025-1
- EN 10025-2
A36
- ASTM A36/A36M
- ASME SA-36
The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.