100Cr6vs52100
EN 100Cr6 (1.3505) and SAE 52100 are almost identical in chemistry: C 0.93–1.05%, Cr 1.35–1.60%. The real difference lies in cleanliness, steelmaking route and inspection requirements. Heat treatment, hardness, uses and ordering notes.
Chemical composition: where they differ
100Cr6 (1.3505) is a high-carbon, chromium-alloyed bearing steel to EN ISO 683-17; 52100 is its counterpart defined in SAE J404 and ASTM A295. Today the chemistry of the two grades overlaps almost exactly: carbon 0.93–1.05%, silicon 0.15–0.35%, manganese 0.25–0.45% and chromium 1.35–1.60%. Phosphorus is limited to 0.025% and sulphur to 0.015%. The difference between 100Cr6 and 52100 is therefore usually not in the chemistry, but in the cleanliness of the steel, the melting and casting route, and the inspections required by the standards or by customer specifications. Japanese SUJ2 and Chinese GCr15 belong to the same family.
Chemical Composition
| Element | 100Cr6 | 52100 |
|---|---|---|
| C | 0.93–1.05 | 0.93–1.05 |
| Si | 0.15–0.35 | 0.15–0.35 |
| Mn | 0.25–0.45 | 0.25–0.45 |
| P | ≤ 0.025 | ≤ 0.025 |
| S | ≤ 0.015 | ≤ 0.015 |
| Cr | 1.35–1.60 | 1.35–1.60 |
Heat (cast) analysis, % by mass.
Basis: 100Cr6 — EN ISO 683-1752100 — SAE J404 / ASTM A295
Mechanical properties and strength
What matters in a bearing steel is not tensile strength but hardness in the hardened condition, rolling-contact fatigue life and dimensional stability. That is why this page has no mechanical table: the standards define hardness in the delivery condition and cleanliness requirements, not strength in service. The usual delivery condition is soft (spheroidise) annealed; in this condition EN ISO 683-17 limits hardness to 207 HB. After hardening and low-temperature tempering, both steels reach about 60–66 HRC. The main factor governing rolling life is non-metallic inclusions, especially oxides; a difference in cleanliness between two heats of the same chemistry can affect life far more than the chemistry does.
Heat treatment and delivery conditions
The process sequence is the same for both grades: spheroidise annealing for a soft, machinable structure, then quenching in oil or polymer from about 830–860 °C and low-temperature tempering at around 150–180 °C. Austenite retained after quenching can transform over time and change dimensions; in precision bearings, dimensional stability is therefore secured by sub-zero treatment or a higher tempering temperature. Bainitic hardening (austempering) is an alternative where less distortion and higher toughness are needed. In heavy-section rings, the hardenability of 100Cr6 may not suffice; grades such as 100CrMo7-3 or 100CrMnSi6-4 from EN ISO 683-17, or on the US side the high-hardenability grades of ASTM A485, are then considered.
Weldability and machinability
With about 1% carbon, neither steel is suitable for welding; hard, crack-prone martensite forms in the heat-affected zone. Machining and cold forming (for example cold heading of balls) are done in the spheroidised soft condition. After hardening, shape is corrected only by grinding, honing and superfinishing; because overheating during grinding can cause surface burn and tensile stresses, the grinding parameters must be controlled.
Typical applications
The main application of 100Cr6 and 52100 is ball and roller bearings: inner and outer rings, balls, rollers and needles. They are also used for precision shafts, ball-screw and linear-guide components, gauges and measuring tools, punches, cold-work tools, pump plungers and wear-resistant pins and bushes. Bearing manufacturers often add their own cleanliness and inspection specifications on top of the standard.
Applications
- Inner and outer bearing rings
- Balls, rollers and needles
- Ball-screw and linear-guide components
- Gauges and measuring tools
- Punches, cold-work tools and wear parts
100Cr6 or 52100: which to choose and when
If the drawing or specification is based on EN, order 100Cr6; if it is of US origin, order 52100. Since the chemistries overlap, the choice is in most cases not technical but a matter of certification and inspection requirements. The real decision parameters are the product form (bar, wire or tube), the delivery condition (spheroidise annealed or as-rolled), the required cleanliness and micro-inclusion class, ultrasonic testing and, if needed, vacuum-degassed steel. For large sections or high core hardness, higher-hardenability bearing steels are considered; where high toughness and impact resistance are needed, case-hardening steels (for example the 16MnCr5 or 8620 family) are considered.
Equivalence caveats and ordering notes
100Cr6 and 52100 are among the EN-ASTM pairs whose chemistry overlaps best; the same heat often satisfies both chemistries. But equivalence is not only chemistry: EN ISO 683-17 and ASTM A295 define inclusion-rating methods, macro and micro cleanliness limits and inspection requirements differently, and ASTM A535 covers special-quality bearing steel with stricter cleanliness requirements. The same applies to SUJ2 and GCr15. In the order, therefore, state together with the grade which standard's cleanliness and inspection requirements apply, the delivery condition and the hardness limit; the inspection certificate (EN 10204 3.1) should show the heat analysis, hardness and, if ordered, the inclusion results.
Grade Equivalents
| System | 100Cr6 | 52100 |
|---|---|---|
| EN | 100Cr6 | ≈ 100Cr6 |
| DIN (W.Nr.) | 1.3505 | ≈ 1.3505 |
| AISI/SAE | ≈ 52100 | 52100 |
| UNS | — | G52986 |
| JIS | ≈ SUJ2 | ≈ SUJ2 |
| GB (China) | ≈ GCr15 | ≈ GCr15 |
Standards
100Cr6
- EN ISO 683-17
52100
- SAE J404
- ASTM A295
- ASTM A535
The values on this page are reference data compiled from the published limits of the standards named. Binding values are those on the material's inspection certificate (EN 10204 3.1), according to the standard and delivery condition stated in the order.
Technical Datasheet
Products made in these grades
Looking for this steel grade?
Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.