Steel Grade Datasheet

X5CrNi18-10/ 1.4301 / 304Austenitic Chromium-Nickel Stainless Steel

Standard
EN 10088-2 / EN 10088-3
Delivery Conditions
+AT
Density
7.90 g/cm³
W.-Nr.
1.4301

What is 1.4301 (AISI 304)?

X5CrNi18-10 (Werkstoff No. 1.4301, AISI 304) is an austenitic stainless steel with 17.5–19.5% chromium and 8.0–10.5% nickel, and the most widely used stainless grade. Solution annealed (+AT), bar has Rp0.2 ≥ 190 MPa, Rm 500–700 MPa and elongation ≥ 45% (EN 10088-3, d ≤ 160 mm). It cannot be hardened by heat treatment, is non-magnetic in the annealed condition and welds well. It is used in atmospheric service and in food and chemical equipment; in chloride-bearing media molybdenum-alloyed 316L (1.4404) is preferred.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C≤ 0.07
Si≤ 1.00
Mn≤ 2.00
P≤ 0.045
S≤ 0.030 (EN 10088-3) · ≤ 0.015 (EN 10088-2)
Cr17.5–19.5
Ni8.0–10.5
N≤ 0.11 (EN 10088:2005)

Mechanical Properties (+AT · EN 10088-3)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 160190500–70045
160 < d ≤ 250190500–70035

Hardness: +AT (solution annealed): ≤ 215 HB (EN 10088-3). Cannot be hardened by heat treatment; it work-hardens during cold forming.

1.4301 / AISI 304 properties and use

1.4301 is the basic austenitic stainless grade in EN 10088-2 (sheet and strip) and EN 10088-3 (bars, wire, sections). Optimum properties are obtained by solution annealing at 1000–1100 °C followed by rapid cooling; strength is raised by cold working, not by heat treatment. With carbon ≤ 0.07% it can become susceptible to intergranular corrosion after welding of heavy sections, because chromium carbides precipitate in the 450–850 °C range; if no solution annealing is possible after welding, low-carbon 1.4307 (304L) is chosen. It is not recommended for seawater or other high-chloride environments. On our site, the flanges (weld neck, slip-on, blind and threaded) and pipe fittings (elbow, tee, reducer) list ASTM A182 F304/F304L among their material options. A182 F304 is the ASTM designation for forged flanges and fittings; it is very close to EN 1.4301 but not identical (e.g. A182 F304 has C ≤ 0.08%, Cr 18.0–20.0%, Ni 8.0–11.0%). The order should therefore state the governing standard and, if needed, dual certification (F304/F304L). For a quotation, state the product type (e.g. flange type and pressure class, fitting type or another form), dimensions, governing standard and quantity. Aktif Çelik reviews the request through its supply network and prepares a quote; the material can be requested with an EN 10204 3.1 inspection certificate. Aktif Çelik supplies 1.4301 / 304 (1.4307 / 304L on request) round, hexagon, square and flat bars to EN 10088-3 or ASTM A276 / A479, from stock or from production partners; stock status for the size, minimum quantity and lead time vary by product and are stated in the quotation. Third-party inspection (e.g. SGS, Bureau Veritas, TÜV) is arranged on request.

Related technical article: X5CrNi18-10

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
ENX5CrNi18-10
W.-Nr. (DIN)1.4301
AISI / UNS304 / S30400
ASTMA182 F304 · A276 · A240
JISSUS304
GOST≈ 08Х18Н10 (08Kh18N10)
AFNORZ7CN18-09 / Z6CN18-09
BS (UK)304S31
GB (China)06Cr19Ni10

Steel Equivalence Tables

Detailed comparison: 304 vs 316L

Applications

  • Food and beverage equipment
  • Mildly corrosive service in chemical and petrochemical plants
  • Flanges, fittings and pipe connection parts
  • Tanks and process vessels
  • Building and architectural applications
  • Kitchen and decorative products

Frequently Asked Questions

Are 304 and 1.4301 the same?+

In practice they are two designations of the same material: AISI 304 is the American name, X5CrNi18-10 / 1.4301 the European one. The ranges are not identical; for example EN 1.4301 has C ≤ 0.07%, whereas ASTM A182 F304 has C ≤ 0.08% and Ni 8.0–11.0%. The certificate states the standard of manufacture; dual-certified material is common.

Is 304 stainless steel magnetic?+

The annealed (solution annealed) austenitic structure is practically non-magnetic. Cold forming such as bending, cold drawing or deep drawing can transform part of the structure into martensite and cause slight magnetism; this does not mean the material is not 304.

What is the difference between 304, 304L and 316L?+

304L (1.4307) is the low-carbon version (≤ 0.030%) and reduces the risk of intergranular corrosion after welding. 316L (1.4404) additionally contains 2.0–2.5% molybdenum and is markedly more resistant to pitting in chloride-containing media. Choose 304L for welded parts and 316L where chlorides (salt, sea air, some chemicals) are present.

Can 1.4301 be hardened?+

No. Austenitic stainless steels do not harden on quenching; strength can only be increased by cold working (work hardening). If high hardness or wear resistance is required, martensitic stainless grades (e.g. 1.4021, 1.4057) are considered.

Does Aktif Çelik supply 304 stainless bars?+

Yes. 1.4301 / 304 (1.4307 / 304L on request) round, hexagon, square and flat bars are supplied with an EN 10204 3.1 certificate. Whether a given size is in stock, the minimum quantity and the lead time are stated in the quotation.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.

Request a Quote

Related Tools

Values on this page are reference data compiled from the applicable EN standard; certified material properties are defined by the mill test certificate (EN 10204 3.1).