42CrMo4 vs 34CrNiMo6 vs 30CrNiMo8: Choosing Q&T Steel by Section Size
In quenched and tempered steel, strength depends on the section size of the part. Using the +QT tables of EN 10083-3, we compare the yield and tensile values of 42CrMo4, 34CrNiMo6 and 30CrNiMo8 from 16 mm up to 250 mm, and we built a selection table that shows the least-alloyed suitable grade for a required yield strength and diameter.
📋 Datasheets: 42CrMo4 → · 34CrNiMo6 → · 30CrNiMo8 → · Overview: Quenched and Tempered Steels Guide
Short Answer
The same strength requires more alloy as the section gets larger. In the quenched and tempered (+QT) condition to EN 10083-3, 42CrMo4 gives a minimum yield of 650 MPa in the 40–100 mm section; at 160–250 mm this falls to 500 MPa. In the same sections 34CrNiMo6 gives 800 and 600 MPa, and 30CrNiMo8 gives 900 and 700 MPa. The right question in grade selection is not "which one is stronger?" but "which grade guarantees the required value at the part's section size?" The answer is the least-alloyed grade that meets the requirement at that section.
Chemistry of the Three Grades
| Element (%) | 42CrMo4 (1.7225) | 34CrNiMo6 (1.6582) | 30CrNiMo8 (1.6580) |
|---|---|---|---|
| C | 0.38–0.45 | 0.30–0.38 | 0.26–0.34 |
| Mn | 0.60–0.90 | 0.50–0.80 | 0.50–0.80 |
| Cr | 0.90–1.20 | 1.30–1.70 | 1.80–2.20 |
| Mo | 0.15–0.30 | 0.15–0.30 | 0.30–0.50 |
| Ni | — | 1.30–1.70 | 1.80–2.20 |
| Closest counterpart | AISI 4140 | ≈ AISI 4340, BS EN24 (817M40) | No exact AISI/SAE counterpart (old AFNOR ≈ 30CND8) |
Source: EN 10083-3; Si ≤ 0.40, P ≤ 0.025, S ≤ 0.035 are common to all three grades.
The trend in the chemistry is clear: carbon goes down while chromium, nickel and molybdenum go up. Carbon sets the maximum hardness that can be reached on quenching. The alloying elements set how deep into the section that hardness can be carried, in other words the hardenability. The values required at the centre of a large shaft are achieved through this second property.
EN 10083-3 +QT Values by Section Band
| Section (d, mm) | 42CrMo4 Re / Rm / A | 34CrNiMo6 Re / Rm / A | 30CrNiMo8 Re / Rm / A |
|---|---|---|---|
| d ≤ 16 | 900 / 1100–1300 / 10 | 1000 / 1200–1400 / 9 | 1050 / 1250–1450 / 9 |
| 16 < d ≤ 40 | 750 / 1000–1200 / 11 | 900 / 1100–1300 / 10 | 1050 / 1250–1450 / 9 |
| 40 < d ≤ 100 | 650 / 900–1100 / 12 | 800 / 1000–1200 / 11 | 900 / 1100–1300 / 10 |
| 100 < d ≤ 160 | 550 / 800–950 / 13 | 700 / 900–1100 / 12 | 800 / 1000–1200 / 11 |
| 160 < d ≤ 250 | 500 / 750–900 / 14 | 600 / 800–950 / 13 | 700 / 900–1100 / 12 |
Re = minimum yield strength (MPa) · Rm = tensile strength (MPa) · A = minimum elongation after fracture (%). Source: EN 10083-3, +QT. Impact energy requirements are given separately in the standard.
The table says three things. First, the yield strength of 42CrMo4 drops by 400 MPa from 16 mm to 250 mm; for 30CrNiMo8 the drop is 350 MPa, and it does not drop at all up to 40 mm. Second, the 700 MPa of 30CrNiMo8 in the 160–250 mm band is higher than the 650 MPa of 42CrMo4 in the 40–100 mm band. Third, elongation rises as the section grows: lower strength comes with more ductility. To convert tensile strength to hardness, use the Hardness Converter tool.
Selection Table: Required Yield × Section
The table below is a selection matrix we derived from the EN 10083-3 values above. Each cell shows the least-alloyed grade that meets the required minimum yield strength at that section. The alloy order is 42CrMo4 → 34CrNiMo6 → 30CrNiMo8. A "—" means none of the three grades guarantees that value at that section.
| Required min. Re | d ≤ 16 | 16–40 | 40–100 | 100–160 | 160–250 |
|---|---|---|---|---|---|
| 500 MPa | 42CrMo4 | 42CrMo4 | 42CrMo4 | 42CrMo4 | 42CrMo4 |
| 600 MPa | 42CrMo4 | 42CrMo4 | 42CrMo4 | 34CrNiMo6 | 34CrNiMo6 |
| 700 MPa | 42CrMo4 | 42CrMo4 | 34CrNiMo6 | 34CrNiMo6 | 30CrNiMo8 |
| 800 MPa | 42CrMo4 | 34CrNiMo6 | 34CrNiMo6 | 30CrNiMo8 | — |
| 900 MPa | 42CrMo4 | 34CrNiMo6 | 30CrNiMo8 | — | — |
| 1000 MPa | 34CrNiMo6 | 30CrNiMo8 | — | — | — |
Basis: EN 10083-3 +QT minimum yield values; only Re is compared. Tensile, elongation, impact and hardenability requirements must be checked separately.
Example: if a Ø180 mm shaft needs a minimum yield of 650 MPa, 42CrMo4 (500 MPa) and 34CrNiMo6 (600 MPa) are not enough; 30CrNiMo8 (700 MPa) is needed. If the same shaft were Ø90 mm, 34CrNiMo6 (800 MPa) would be more than enough, and even 42CrMo4 would just meet the 650 MPa limit. The gaps in the table are a message too. If 800 MPa yield is required at Ø200 mm, the answer is not a higher alloy but a smaller section: rough-machine first and then quench and temper, or change the design.
What Does "Section" Mean? The Point Often Missed on Orders
The "d" in the standard is the ruling section during heat treatment: the diameter for a round bar, the thickness for a flat. The values are guaranteed on test pieces taken from a position defined by the standard (EN ISO 377), not from the centre. Because the centre of a thick section cools more slowly, the strength at the centre can be below the table value.
Practical consequences:
- Part machined after quenching and tempering: If a Ø200 mm bar is quenched and tempered and then turned to Ø120 mm, the part's values are read from the Ø200 mm band, not the Ø120 mm band.
- Part rough-machined first, then quenched and tempered: The material is bought soft annealed (+A), machined close to the final section, then quenched and tempered. This way a smaller section band applies. For delivery condition codes, see our delivery condition guide.
- If centre values are critical (heavy shaft, crankshaft, gear hub), the test piece position and value must be stated separately on the order.
What Nickel and Molybdenum Do
What separates 34CrNiMo6 and 30CrNiMo8 from 42CrMo4 is nickel. Nickel increases hardenability while preserving toughness, which is why these grades are chosen for large parts under impact loading. The higher molybdenum in 30CrNiMo8 (0.30–0.50) increases hardenability and provides resistance to temper embrittlement during tempering. There is a price: nickel and molybdenum are expensive alloying elements, high hardenability makes welding harder, and because 30CrNiMo8 has no exact US counterpart, buyers looking for an equivalent turn to the 4340 class. The relationship between 34CrNiMo6 and AISI 4340 is covered in our 34CrNiMo6 vs 4340 comparison; international equivalents are in the Grade Equivalent tool.
Above 250 mm: The Forging Standard
The EN 10083-3 tables end at 250 mm. For forged shafts and blocks with larger sections, values are tabulated separately in the open-die forging standard EN 10250-3, and are often agreed with the manufacturer on the order. At these sizes, forging ratio, ultrasonic testing and test piece position matter as much as the grade name. We explain the difference between forged and rolled bar in our forged vs rolled article.
Which One to Choose?
Choose 42CrMo4 if:
- The section is up to about Ø100 mm and the yield requirement is around 650 MPa
- The part will be nitrided or induction surface hardened
- A wide size range and easy availability matter
Choose 34CrNiMo6 if:
- The section is in the 100–250 mm range and 600–700 MPa yield is required
- Impact and fatigue loads are heavy and toughness is the priority
- The specification calls for a material in the AISI 4340 / EN24 class
Choose 30CrNiMo8 if:
- 700 MPa yield or more is required at a large section (160–250 mm)
- Very high strength is required, such as 1050 MPa yield up to 40 mm
- You are in heavy machinery, energy or defence applications with high safety factors
What to Write in the Specification
- Grade and standard:
34CrNiMo6, EN 10083-3 - Delivery condition: +A (if it will be quenched and tempered later) or +QT (quenched and tempered bar); +H for a hardenability band if you will heat treat it yourself
- Size and form: diameter × length; rolled, forged or bright (peeled) bar
- Mechanical requirement: required Re / Rm / impact value and the test piece position (if centre values are critical)
- Inspection: ultrasonic testing for large diameters (EN 10308 for bars, EN 10228-3 for forgings)
- Documents: EN 10204 3.1; third-party inspection by SGS, Bureau Veritas or TÜV if required. To check the certificate, see our 3.1 certificate guide.
Frequently Asked Questions
Can 42CrMo4 be used instead of 34CrNiMo6?
It depends on the section. At 16–40 mm, 42CrMo4 gives 750 MPa yield and 34CrNiMo6 900 MPa; if your requirement is 750 MPa, 42CrMo4 is enough. Above 100 mm the gap widens and 42CrMo4 usually cannot replace 34CrNiMo6.
What is the difference between 30CrNiMo8 and 34CrNiMo6?
30CrNiMo8 contains more chromium, nickel and molybdenum. In EN 10083-3 it gives 50–150 MPa more yield strength than 34CrNiMo6 in every section band. At 160–250 mm the difference is 700 versus 600 MPa.
Which grade for a Ø300 mm shaft?
The EN 10083-3 tables end at 250 mm. At this size the part is usually ordered as a forging, and the values are set by EN 10250-3 or by agreement with the manufacturer. 34CrNiMo6 and 30CrNiMo8 are frequently used grades at these sizes.
Are 34CrNiMo6 and AISI 4340 the same steel?
They are close counterparts, not identical. The chemistry ranges and the standards defining the mechanical values differ. The governing standard must be stated clearly on the order.
Sourcing from Aktif Çelik
We supply 42CrMo4, 34CrNiMo6 and 30CrNiMo8 as forged bar, hot rolled bar and bright (peeled) bar, in the +A or +QT condition and with an EN 10204 3.1 inspection certificate. Tell us the part diameter, the required mechanical values and where the heat treatment will be done; we will confirm the right grade for the section band together with the manufacturers in our supply network. Quotes are sent within 24 hours; size, quantity and lead time are confirmed in the quote.
🔗 See also: Steel Equivalence Tables · Quality & Certificates
Detailed Technical Info & Quotation
Contact our expert team for detailed technical documents, application recommendations, and custom dimension quotes on this topic.