Steel Grade Datasheet

C60/ 1.0601 / ≈ 1060High-Carbon Steel for Quenching and Tempering

Standard
EN 10083-2
Delivery Conditions
+A, +N, +QT
Density
7.85 g/cm³
W.-Nr.
1.0601

What is C60 steel?

C60 (material no. 1.0601) is the highest-carbon non-alloy steel for quenching and tempering in EN 10083-2, with 0.57–0.65% carbon and 0.60–0.90% manganese. Quenched and tempered (+QT), it reaches a minimum yield strength of 580 MPa and 850–1000 MPa tensile strength up to 16 mm, and 450 MPa / 750–900 MPa for 40–100 mm. It is used where strength and wear resistance matter more than toughness and weldability.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C0.57–0.65
Si≤ 0.40
Mn0.60–0.90
P≤ 0.045 (C60E/C60R ≤ 0.030)
S≤ 0.045 (C60E ≤ 0.035; C60R 0.020–0.040)
Cr≤ 0.40
Mo≤ 0.10
Ni≤ 0.40
Cr+Mo+Ni≤ 0.63

Mechanical Properties (+QT)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16580850–100011
16 < d ≤ 40520800–95013
40 < d ≤ 100450750–90014

Mechanical Properties (+N)

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16380≥ 71010
16 < d ≤ 100340≥ 67011
100 < d ≤ 250310≥ 65011

Hardness: +QT: Rm 750–1000 MPa ≈ 220–295 HB · +N: Rm ≥ 650–710 MPa · HB values are an approximate conversion per EN ISO 18265; EN 10083-2 specifies strength, not hardness, for +N/+QT.

C60 / 1.0601 properties and use

Its high carbon content gives C60 the highest strength and wear resistance of the series, while toughness and elongation are the lowest (+QT up to 16 mm: A ≥ 11%). As a non-alloy steel its hardenability is limited, and the EN 10083-2 values fall markedly as the section grows. For large sections or highly stressed springs, an alloy steel such as 51CrV4 is the better choice. EN 10083-2 also defines C60E (1.1221; old DIN name Ck60) and C60R (1.1223, sulphur 0.020–0.040%) with the same mechanical values. Guideline heat treatment: normalizing at about 820–860 °C, hardening from about 800–840 °C in oil or water (oil is usual for complex shapes to limit the risk of cracking), tempering at 550–660 °C for strength; lower tempering temperatures give higher hardness. Welding C60 is generally not recommended; where it cannot be avoided, preheating and post-weld heat treatment must follow a qualified procedure. Machining is usually done in the soft annealed (+A) or normalized (+N) condition. Aktif Çelik quotes C60 through its supply network as hot-rolled bar and as forgings; size, delivery condition, quantity and lead time are confirmed in the quotation, and deliveries can be made with an EN 10204 3.1 inspection certificate.

Related technical article: C60

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
ENC60
W.-Nr. (DIN)1.0601
EN (E / R)C60E 1.1221 / C60R 1.1223
DIN 17200 (old)Ck60 (= C60E)
AISI/SAE≈ 1060
JIS≈ S58C
GOST≈ 60 (сталь 60)
GB (China)≈ 60

Steel Equivalence Tables

Applications

  • Wear-resistant parts such as rollers, cams and guides
  • Simple, low-stressed springs and spring washers
  • Wear parts for agricultural and earth-moving machinery
  • Shafts and spindles with induction-hardened bearing surfaces
  • Coupling and clutch components
  • Hand tools and clamping elements

Frequently Asked Questions

What is the difference between C60 and C45?+

C60 contains 0.57–0.65% carbon, C45 0.42–0.50%. Quenched and tempered up to 16 mm, C60 gives 850–1000 MPa and C45 700–850 MPa tensile strength, while elongation is 11% for C60 and 14% for C45. C60 is harder and more wear-resistant but less tough, and it is harder to weld and machine.

Is C60 weldable?+

Welding is generally not recommended: the high carbon content creates a hard, brittle heat-affected zone and a risk of cracking. If welding cannot be avoided, preheating, controlled cooling and post-weld heat treatment must follow a qualified welding procedure.

Can C60 be used as spring steel?+

It is used for simple, low-stressed springs and spring clips. For highly stressed and fatigue-loaded springs, chromium-vanadium spring steels such as 51CrV4 are preferred because of their higher hardenability and fatigue strength.

What are the equivalents of C60?+

AISI/SAE 1060, JIS S58C, GOST steel 60 and Chinese 60 are close matches but not identical: GOST 60, for example, specifies 0.50–0.80% Mn versus 0.60–0.90% in C60, and JIS S58C has 0.55–0.61% C. The old DIN grade Ck60 corresponds to today's C60E.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.