Steel Grade Datasheet

C55/ 1.0535 / ≈ 1055Non-Alloy Q&T Steel (EN 10083-2)

Standard
EN 10083-2
Delivery Conditions
+A, +N, +QT
Density
7.85 g/cm³
W.-Nr.
1.0535

What is C55 steel?

C55 (material no. 1.0535) is a non-alloy steel for quenching and tempering to EN 10083-2 with 0.52–0.60% carbon. It has the variants C55E (1.1203, formerly Ck55) with controlled phosphorus and sulphur and C55R (1.1209, formerly Cm55) with a defined sulphur range. Quenched and tempered (+QT), it gives a minimum yield strength of 550 MPa and a tensile strength of 800–950 MPa up to 16 mm; normalized (+N), min. 370 MPa yield and min. 680 MPa tensile strength up to 16 mm. It is used for shafts, gears and induction-hardened parts that need more strength and wear resistance than C45.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C0.52–0.60
Si≤ 0.40
Mn0.60–0.90
P≤ 0.045 (C55E/C55R ≤ 0.030)
S≤ 0.045 (C55E ≤ 0.035; C55R 0.020–0.040)
Cr≤ 0.40
Mo≤ 0.10
Ni≤ 0.40
Cr+Mo+Ni≤ 0.63

Mechanical Properties (+QT)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16550800–95012
16 < d ≤ 40490750–90014
40 < d ≤ 100420700–85015

Mechanical Properties (+N)

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16370≥ 68011
16 < d ≤ 100330≥ 64012
100 < d ≤ 250300≥ 62012

Hardness by Delivery Condition

Hardness limits given by the standard for these delivery conditions; certified values are stated on the inspection certificate (EN 10204 3.1).

Delivery conditionHardness
+A≤ 229 HB

Hardness: +A: max. 229 HB (EN 10083-2) · +QT: Rm 700–950 MPa ≈ 205–280 HB · +N: Rm ≥ 620–680 MPa ≈ 180–200 HB and above (HB values are an approximate conversion per EN ISO 18265).

C55 / 1.0535 properties and use

Among the carbon steels of EN 10083-2, C55 sits between C45 and C60. Higher carbon gives more strength than C45 in the same section and a higher surface hardness after flame or induction hardening, while toughness and weldability fall. As a non-alloy steel its hardenability is limited: the standard gives +QT values only up to 100 mm, and strength drops quickly with section (minimum yield 550 MPa up to 16 mm, 420 MPa at 40–100 mm). Where large sections need high core strength, an alloy Q&T steel such as 42CrMo4 is chosen. Typical heat treatment (guide values from producer datasheets): normalizing at 825–865 °C, soft annealing at 680–710 °C, hardening at 805–845 °C in oil or water, tempering at 550–660 °C. For machining it can be ordered in the +A condition (soft annealed, max. 229 HB). Welding is not recommended; where unavoidable, preheating and post-weld stress relieving are required. Name conversion: C55E replaces Ck55 of the old DIN 17200, and C55R replaces Cm55. Aktif Çelik supplies C55 / C55E as hot-rolled round and flat bars and as cold-drawn (bright) bars, from stock or through its production partners depending on size and quantity; whether a given size is in stock, the delivery condition, the minimum quantity and the lead time are stated in the quotation. Deliveries come with an EN 10204 3.1 inspection certificate; third-party inspection by bodies such as SGS, Bureau Veritas or TÜV can be arranged on request.

Related technical article: C55

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
ENC55
W.-Nr. (DIN)1.0535
EN (E / R)C55E 1.1203 / C55R 1.1209
DIN 17200 (old)Ck55 (= C55E) / Cm55 (= C55R)
AISI/SAE≈ 1055
JIS≈ S55C
GOST≈ 55 (сталь 55)
BS 970 (UK)≈ 070M55 (EN9)
GB (China)≈ 55

Steel Equivalence Tables

Applications

  • Shafts, axles and spindles
  • Induction- or flame-hardened gears, sprockets and racks
  • Rolls, rollers and guide rails
  • Cutting and wear parts in agricultural machinery
  • Machine parts needing more wear resistance than C45
  • Hand tools and forged parts

Frequently Asked Questions

What is the difference between C55, C45 and C60?+

The difference is carbon content: 0.42–0.50% in C45, 0.52–0.60% in C55 and 0.57–0.65% in C60. Under EN 10083-2 the minimum +QT yield strength up to 16 mm is 490 MPa for C45, 550 MPa for C55 and 580 MPa for C60. As carbon rises, strength and the hardness reached in surface hardening increase, while toughness, weldability and formability decrease. C55 is the middle option where C45 is not enough but the lower toughness of C60 is not wanted.

What is the difference between C55, C55E and C55R?+

All three have the same carbon range and mechanical values; the difference lies in the phosphorus and sulphur limits. C55 allows max. 0.045% P and S. C55E (1.1203, formerly Ck55) has max. 0.030% P and max. 0.035% S and is preferred for more uniform results in hardening and surface hardening. C55R (1.1209, formerly Cm55) keeps S within 0.020–0.040% to improve machinability.

What are the AISI and GOST equivalents of C55?+

The nearest equivalents are AISI/SAE 1055, JIS S55C, GOST 1050 steel 55 and British BS 970 070M55 (EN9). Carbon ranges are very close, but some element limits such as manganese and the mechanical requirements are defined by different standards, so the table shows them with '≈'. Any substitution should be approved after comparing the order standard.

Can C55 be welded?+

Because of its high carbon it is not a grade for welding; a hard, crack-prone structure can form in the heat-affected zone. If welding is unavoidable, suitable preheating, low-hydrogen filler metal and post-weld stress relieving are needed, and the procedure should be set by a welding engineer. For welded structures, structural steels such as S355J2 are preferred.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.

Request a Quote

Related Tools

Values on this page are reference data compiled from the applicable EN standard; certified material properties are defined by the mill test certificate (EN 10204 3.1).