Steel Grade Datasheet

34CrMo4/ 1.7220 / ≈ 4135Chromium-Molybdenum Steel for Quenching and Tempering

Standard
EN 10083-3
Delivery Conditions
+A, +QT
Density
7.85 g/cm³
W.-Nr.
1.7220

What is 34CrMo4 steel?

34CrMo4 (material no. 1.7220) is a chromium-molybdenum alloy steel for quenching and tempering to EN 10083-3, with 0.30–0.37% carbon, 0.90–1.20% chromium and 0.15–0.30% molybdenum. Quenched and tempered (+QT), it offers a minimum yield strength of 800 MPa and 1000–1200 MPa tensile strength up to 16 mm; the standard gives values up to 250 mm (160–250 mm: 450 MPa / 700–850 MPa). It is the lower-carbon, tougher sibling of 42CrMo4.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C0.30–0.37
Si≤ 0.40
Mn0.60–0.90
P≤ 0.025
S≤ 0.035 (34CrMoS4: 0.020–0.040)
Cr0.90–1.20
Mo0.15–0.30

Mechanical Properties (+QT)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 168001000–120011
16 < d ≤ 40650900–110012
40 < d ≤ 100550800–95014
100 < d ≤ 160500750–90015
160 < d ≤ 250450700–85015

Hardness: +QT: Rm 700–1200 MPa ≈ 205–355 HB · HB values are an approximate conversion per EN ISO 18265; EN 10083-3 specifies strength, not hardness, for +QT · +A (soft annealed) for machining.

34CrMo4 / 1.7220 properties and use

34CrMo4 shares the chromium-molybdenum alloy system of 42CrMo4 but has less carbon. This makes it tougher and somewhat more suitable for welding, while its maximum strength is a little below 42CrMo4. Molybdenum raises hardenability and provides resistance to temper embrittlement, which is why EN 10083-3 specifies 34CrMo4 values up to 250 mm. It is widely used for shafts, gears and fasteners that need strength together with toughness, and for seamless pressure gas cylinders (to the cylinder standard's own material requirements). Machining is done in the soft annealed (+A) condition; 34CrMoS4 (1.7226), with sulphur held at 0.020–0.040%, improves machinability. Guideline heat treatment: hardening from about 830–870 °C in water or oil and tempering at 540–680 °C. Induction hardening of the surface is also possible. Welding is conditional: preheating, low-hydrogen consumables and, where required, post-weld heat treatment must be set in a qualified procedure. Aktif Çelik quotes 34CrMo4 through its supply network as hot-rolled round bar, bright (peeled or cold-drawn) bar and as forgings; size, delivery condition, quantity and lead time are confirmed in the quotation, and deliveries can be made with an EN 10204 3.1 inspection certificate.

Related technical article: 34CrMo4

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
EN34CrMo4
W.-Nr. (DIN)1.7220
EN (S)34CrMoS4 1.7226
AISI/SAE≈ 4135 / 4137
JIS≈ SCM435
GOST≈ 35ХМ (35KhM)
AFNOR (old)≈ 34CD4
BS 970 (UK)≈ 708A37
GB (China)≈ 35CrMo

Steel Equivalence Tables

Applications

  • Shafts, axles and gear shafts
  • Gears and couplings
  • High-strength bolts and studs
  • Seamless pressure gas cylinders
  • Automotive driveline and axle parts
  • Forgings for machinery and power transmission

Frequently Asked Questions

What is the difference between 34CrMo4 and 42CrMo4?+

34CrMo4 has 0.30–0.37% carbon, 42CrMo4 0.38–0.45%; the chromium and molybdenum ranges are the same. Quenched and tempered up to 16 mm, 34CrMo4 gives 800 MPa yield / 1000–1200 MPa and 42CrMo4 900 MPa / 1100–1300 MPa. 34CrMo4 is tougher and more weld-friendly; 42CrMo4 is chosen when maximum strength is needed. Both have values defined up to 250 mm.

Is 34CrMo4 the same as AISI 4135/4137 and SCM435?+

Close, but not identical. JIS SCM435 is the nearest match in composition. AISI 4135 and 4137 are similar CrMo steels with slightly different carbon, manganese and chromium ranges, and GOST 35KhM (35ХМ) specifies lower manganese (0.40–0.70%). For certified supply, the standard named in the order governs.

Can 34CrMo4 be welded?+

Conditionally, yes. Because of its alloy and carbon content, preheating and low-hydrogen consumables are needed against cold cracking, with post-weld stress relieving where required. Parameters should be set in a qualified welding procedure.

In which delivery conditions is 34CrMo4 available?+

EN 10083-3 allows delivery untreated, treated for shearability (+S), soft annealed (+A) or quenched and tempered (+QT). Choose +A for machining and +QT for direct use; if machinability matters, the 34CrMoS4 variant can be specified.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.

Request a Quote

Related Tools

Values on this page are reference data compiled from the applicable EN standard; certified material properties are defined by the mill test certificate (EN 10204 3.1).