Steel Grade Datasheet

38MnVS6/ 1.1303Microalloyed Forging Steel (EN 10267)

Standard
EN 10267
Delivery Conditions
+P
Density
7.85 g/cm³
W.-Nr.
1.1303

What is 38MnVS6 steel?

38MnVS6 (material no. 1.1303) is a vanadium-microalloyed, precipitation-hardening ferritic-pearlitic steel (AFP steel) to EN 10267. Cooled in a controlled way in air from the forging temperature (+P), it reaches a minimum yield strength of 520 MPa and a tensile strength of 800–950 MPa without separate quenching and tempering. It contains 0.34–0.41% carbon, 1.20–1.60% manganese, 0.08–0.20% vanadium and 0.020–0.060% sulphur for machinability. It is an economical alternative to Q&T steels for automotive forgings such as crankshafts, connecting rods and steering knuckles.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C0.34–0.41
Si0.15–0.80
Mn1.20–1.60
P≤ 0.025
S0.020–0.060
Cr≤ 0.30
Mo≤ 0.08
V0.08–0.20
N0.010–0.020

Mechanical Properties (+P)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
—520800–95012

Hardness: +P: Rm 800–950 MPa ≈ 235–280 HB (approximate conversion per EN ISO 18265; EN 10267 specifies strength, not hardness). Values in the part depend on the cooling conditions.

38MnVS6 / 1.1303 properties and use

In AFP (precipitation-hardening ferritic-pearlitic) steels, strength comes from fine vanadium carbonitrides that precipitate in the ferrite-pearlite structure during controlled cooling after forging. This removes the quenching, tempering and straightening steps of Q&T steels, saves energy and time, and avoids quench distortion and cracking. In return, toughness is lower than that of quenched and tempered Cr-Mo steels of the same strength, so Q&T steels such as 42CrMo4 are preferred for parts with high impact loads. The mechanical values of EN 10267 (Rp0.2 min. 520 MPa, Rm 800–950 MPa, elongation min. 12%, reduction of area min. 25%) apply to the +P condition, controlled-cooled from the forging temperature; actual values in the part depend on forging temperature, section and cooling rate. Bar for forging is usually delivered hot rolled and untreated, and the forge controls the cooling conditions. Controlled sulphur improves machinability; surfaces such as crankshaft journals are induction hardened where required. 30MnVS6 and 46MnVS6 in the same standard offer other strength levels. Aktif Çelik supplies 38MnVS6 as forging stock in hot-rolled round and square bars, from stock or through its production partners depending on size and quantity; whether a given size is in stock, the minimum quantity and the lead time are stated in the quotation. Deliveries come with an EN 10204 3.1 inspection certificate; third-party inspection by bodies such as SGS, Bureau Veritas or TÜV can be arranged on request.

Related technical article: 38MnVS6

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
EN38MnVS6
W.-Nr. (DIN)1.1303

Steel Equivalence Tables

Applications

  • Crankshafts
  • Connecting rods
  • Steering knuckles and stub axles
  • Steering arms
  • Wheel hubs
  • Piston crowns and other automotive forgings

Frequently Asked Questions

What is an AFP steel, and why does 38MnVS6 need no quenching and tempering?+

AFP stands for precipitation-hardening ferritic-pearlitic steel. The vanadium in 38MnVS6 precipitates as fine carbonitrides during controlled air cooling after forging and strengthens the ferrite-pearlite structure. The part therefore reaches the 800–950 MPa tensile strength of EN 10267 without a separate quench and temper. The condition is that forging temperature and cooling rate are controlled in the process.

What is the difference between 38MnVS6 and C45 or 42CrMo4?+

38MnVS6 is used in forgings that would otherwise be made from quenched and tempered carbon steels such as C45, to remove the Q&T step; its toughness is lower than that of Q&T steels. Quenched and tempered 42CrMo4 gives higher strength and toughness. Where high impact loads, large sections or low service temperatures are involved, a Q&T steel is chosen; the choice should follow the load profile of the part and validation tests.

Is there an AISI, GOST or JIS equivalent of 38MnVS6?+

There is no exact equivalent. 38MnVS6 is an AFP grade of the European standard EN 10267; microalloyed forging steels in other systems are defined with different compositions and requirements. If a similar grade is to be used, chemical composition and as-forged mechanical values should be compared and approved by an engineer.

Can 38MnVS6 be machined and welded?+

Thanks to its controlled sulphur (0.020–0.060%), machinability is good. It is not a grade for welding: carbon and manganese can form a hard structure in the heat-affected zone, and the welding heat locally changes the strength gained by precipitation hardening. If welding is needed, the procedure should be qualified by trials beforehand.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.