Steel Grade Datasheet

C22E/ 1.1151 / ≈ 1020Low-Carbon Non-Alloy Special Steel

Standard
EN 10083-2
Delivery Conditions
+A, +N, +QT
Density
7.85 g/cm³
W.-Nr.
1.1151

What is C22E steel?

C22E (material no. 1.1151) is a low-carbon non-alloy special steel to EN 10083-2 with 0.17–0.24% carbon, 0.40–0.70% manganese and limited phosphorus (≤ 0.030%) and sulphur (≤ 0.035%). Normalized (+N), it offers a minimum yield strength of 240 MPa and tensile strength of at least 430 MPa up to 16 mm; quenched and tempered (+QT), it reaches 500–650 MPa up to 16 mm. Good weldability and formability make it suitable for welded, forged and case-hardened parts with moderate strength requirements.

Chemical Composition

Cast analysis, % by weight (per the applicable EN standard)

ElementRange (%)
C0.17–0.24
Si≤ 0.40
Mn0.40–0.70
P≤ 0.030
S≤ 0.035
Cr≤ 0.40
Mo≤ 0.10
Ni≤ 0.40
Cr+Mo+Ni≤ 0.63

Mechanical Properties (+QT)

Values depend on ruling section / thickness (d).

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16340500–65020
16 < d ≤ 40290470–62022

Mechanical Properties (+N)

Section (mm)Yield Re min (MPa)Tensile Rm (MPa)Elongation A min (%)
d ≤ 16240≥ 43024
16 < d ≤ 100210≥ 41025
100 < d ≤ 250210≥ 40025

Hardness: +QT: Rm 470–650 MPa ≈ 140–195 HB · +N: Rm ≥ 400–430 MPa · HB values are an approximate conversion per EN ISO 18265; EN 10083-2 specifies strength, not hardness, for +N/+QT.

C22E / 1.1151 properties and use

Its low carbon content gives C22E good weldability and cold formability. The strength that can be gained by quenching and tempering is limited: EN 10083-2 gives +QT values only up to 40 mm, and in larger sections the hardening effect is weak. C22E is therefore mostly used in the normalized condition. Its surface can be carburized to produce a wear-resistant case; this suits parts with modest core-strength requirements — where higher core strength is needed, alloyed case-hardening steels such as 16MnCr5 are chosen. EN 10083-2 lists three versions: the quality steel C22 (1.0402) with phosphorus and sulphur up to 0.045%; the special steel C22E (1.1151, old DIN name Ck22) with tighter P and S limits; and C22R (1.1149) with sulphur controlled at 0.020–0.040% for machinability. Guideline heat treatment: normalizing at about 880–920 °C, hardening from about 860–900 °C in water, tempering at 550–660 °C. C22E must not be confused with C22.8, which appears in flange and pressure-vessel forgings: C22.8 (1.0460) is the pressure-equipment forging grade of DIN 17243 and is covered today by P250GH in EN 10222-2. Aktif Çelik quotes C22E through its supply network as hot-rolled and bright bar and as forgings; size, delivery condition, quantity and lead time are confirmed in the quotation, and deliveries can be made with an EN 10204 3.1 inspection certificate.

Related technical article: C22E

International Equivalents

Values marked ≈ are nearest matches, not exact equivalents. Always confirm against the governing standard.

SystemGrade
ENC22E
W.-Nr. (DIN)1.1151
EN (base / R)C22 1.0402 / C22R 1.1149
DIN 17200 (old)Ck22
AISI/SAE≈ 1020
JIS≈ S20C
GOST≈ 20 (сталь 20)
BS 970 (UK)≈ 070M20 (EN3B)
GB (China)≈ 20

Steel Equivalence Tables

Applications

  • Welded machine and frame components
  • Forgings for general mechanical engineering
  • Case-hardened pins and bushes with modest core-strength needs
  • Cold-formed and machined parts
  • Levers, hubs and couplings
  • Lightly stressed shafts and axles

Product pages for this grade

Frequently Asked Questions

What is the difference between C22, C22E and C22R?+

All three share the same base analysis (0.17–0.24% C) and the same mechanical values. C22 (1.0402) is a quality steel with P and S up to 0.045%. C22E (1.1151) is a special steel with P ≤ 0.030% and S ≤ 0.035%; its old DIN name is Ck22. C22R (1.1149) contains 0.020–0.040% sulphur for better chip breaking.

Is C22E weldable?+

Yes. Thanks to its low carbon content it welds well, usually without preheating at normal thicknesses. For thick sections and highly restrained joints, preheating should be set in the welding procedure according to the carbon equivalent.

Is C22E the same as C22.8 or P250GH?+

No. C22.8 (1.0460) is the forging grade for pressure equipment to DIN 17243 and is covered today by P250GH in EN 10222-2, which specifies elevated-temperature and impact requirements. For pressure parts such as flanges, C22E must not replace that grade without design approval.

What are the equivalents of C22E?+

AISI 1020, JIS S20C, GOST steel 20 and BS 970 070M20 (EN3B) are the nearest matches, but not identical. GOST steel 20, for example, specifies 0.17–0.24% C and 0.35–0.65% Mn, and AISI 1020 0.18–0.23% C and 0.30–0.60% Mn. The old DIN name is Ck22.

Looking for this steel grade?

Request a quote with your sizes, tolerances and delivery condition — we respond within 24 hours.

Request a Quote

Related Tools

Values on this page are reference data compiled from the applicable EN standard; certified material properties are defined by the mill test certificate (EN 10204 3.1).